Deposition examples
See examples of depositions that combine anti-reflection and antifouling coatings
1 OS-50, SiO2(E), SURFCLEAR 100
Film Structure
Evaporation material |
Target thickness[nm] |
|
|---|---|---|
| Substrate | BK7 | ― |
| First layer | SiO2(E) | 20 |
| Second layer | OS-50 | 14 |
| Third layer | SiO2(E) | 33 |
| Fourth layer | OS-50 | 111 |
| Fifth layer | SiO2(E) | 83 |
| Sixth layer | SURFCLEAR 100(M) | 12~14 |
| Air | ― | ― |
* Films deposited on one side of substrat
Measurement Results
Spectroscopic Characteristics
Fig. 6 Spectroscopic Characteristics (Transmittance + Reflectance) of AR + AF Coating
Fig. 7 Spectroscopic Characteristics (Transmittance) of AR + AF Coating
Fig. 8 Spectroscopic Characteristics (Reflectance/Both Sides Polished) of AR + AF Coating
Fig. 9 Spectroscopic Characteristics (Reflectance/One Side Polished) of AR + AF Coating
Evaluation of Contact Angle for Water |
|
|---|---|
| Contact angle | 117[deg.] |
Pure water
2.5 μ L , average of 5 measurements
Abrasion Resistance Test |
|
|---|---|
| NG abrasion resistance times | 3000~4000 [times] |
Abrasion material:Steel wool #0000 Load :1000 [g]
2 OH-14, SiO2(E), SURFCLEAR 100
Film Structure
Evaporation material |
Target thickness[nm] |
|
|---|---|---|
| Substrate | BK7 | ― |
| First layer | SiO2(E) | 15 |
| Second layer | OH-14(A) | 16.5 |
| Third layer | SiO2(E) | 35 |
| Fourth layer | OH-14(A) | 136.5 |
| Fifth layer | SiO2(E) | 91 |
| Sixth layer | SURFCLEAR 100(M) | 12–14 |
| Air | ― | ― |
* Films deposited on one side of substrate
Measurement Results
Spectroscopic Characteristics
Fig. 6 Spectroscopic Characteristics (Transmittance + Reflectance) of AR + AF Coating
Fig. 7 Spectroscopic Characteristics (Transmittance) of AR + AF Coating
Fig. 8 Spectroscopic Characteristics (Reflectance/Both Sides Polished) of AR + AF Coating
Fig. 9 Spectroscopic Characteristics (Reflectance/One Side Polished) of AR + AF Coating
Evaluation of Contact Angle for Water |
|
|---|---|
| Contact angle | 117[deg.] |
Pure water
2.5 μ L , average of 5 measurements
Abrasion Resistance Test |
|
|---|---|
| NG abrasion resistance times | 3000~5000 [times] |
Abrasion material:Steel wool #0000 Load :1000 [g]
3 De-gas Nb2O5, SiO2(E), SURFCLEAR 100
Film Structure
Evaporation material |
Target thickness[nm] |
|
|---|---|---|
| Substrate | BK7 | ― |
| First layer | SiO2(E) | 20 |
| Second layer | DegassedNb2O5 | 15 |
| Third layer | SiO2(E) | 36 |
| Fourth layer | DegassedNb2O5 | 120 |
| Fifth layer | SiO2(E) | 86 |
| Sixth layer | SURFCLEAR 100(M) | 12~14 |
| Air | ― | ― |
* Films deposited on one side of substrate
Please contact us here for deposition conditions, measurement conditions, and other detailed information.
Measurement Results
Spectroscopic Characteristics
Fig. 6 Spectroscopic Characteristics (Transmittance + Reflectance) of AR + AF Coating
Fig. 7 Spectroscopic Characteristics (Transmittance) of AR + AF Coating
Fig. 8 Spectroscopic Characteristics (Reflectance/Both Sides Polished) of AR + AF Coating
Fig. 9 Spectroscopic Characteristics (Reflectance/One Side Polished) of AR + AF Coating
Evaluation of Contact Angle for Water |
|
|---|---|
| Contact angle | 117[deg.] |
Pure water
2.5 μ L , average of 5 measurements
Abrasion Resistance Test |
|
|---|---|
| NG abrasion resistance times | 3000~4000 [times] |
brasion material:Steel wool #0000 Load :1000 [g]
Please contact us here for deposition conditions, measurement conditions, and other detailed information.